| Elementum offensionis 8011 |
Content (%) |
| aluminium |
≥98.5 |
| Pii (Si) |
0.5-0.9 |
| Ferrum (Fe) |
0.6-1.0 |
| Aeris (Cu) |
≤0.15 |
| Manganese (Mn) | ≤0.10 |
| Magnesium (Mg) | ≤0.05 |
| Zinc(Zn) | ≤0.10 |
| Aliae immunitates | ≤0.15(total) |
| Proprietas offensionis 8011 |
Ingenium: O |
Ingenium: 12 | Ingenium: 14 | Ingenium: 16 | Ingenium: 18 |
| distrahentes Fortitudo |
90-130 MPa |
110-150 MPa | 130-170 MPa | 150-190 MPa | ≥170 MPa |
| Cede fortitudo (0.2% offset) |
35-65 MPa |
65-105 MPa | 95-135 MPa | 125-165 MPa | ≥150 MPa |
| Elongation at Break |
18-25% |
8-14% | 6-12% | 4-10% | 3-8% |
| Duritia (Rockwell B) |
25-40 |
40-55 | 50-70 | 60-80 | 70-90 |
| Proprietas offensionis 8011 |
Precium |
| Density |
2.7 g/cm³ |
| Liquefactio Point |
643-657°C |
| Scelerisque Conductivity |
209 W/m·K |
| Electrical Conductivity |
61% IACS |
| Scelerisque Expansion Coefficient |
23.1×10⁻⁶/°C (20–100°C) |
| ASTM |
B209 (sheet/plate), B221 (extrusiones), B233 (filum), B479 (foil). |
| ISO |
ISO 26204 (vocabula stannum), ISO 6892 (probatio mechanica). |
| UNS |
A91060 (United States Numbering System). |