| Elemento ng haluang metal 8011 |
Nilalaman (%) |
| Aluminyo (Al) |
≥98.5 |
| Silicon (Si) |
0.5-0.9 |
| Bakal (Fe) |
0.6-1.0 |
| Copper(Cu) |
≤0.15 |
| Manganese(Mn) | ≤0.10 |
| Magnesium(Mg) | ≤0.05 |
| Sink(Zn) | ≤0.10 |
| Iba pang mga Impurities | ≤0.15(kabuuan) |
| Ari-arian ng haluang metal 8011 |
Galit: O |
Galit: 12 | Galit: 14 | Galit: 16 | Galit: 18 |
| Lakas ng makunat |
90-130 MPa |
110-150 MPa | 130-170 MPa | 150-190 MPa | ≥170 MPa |
| Lakas ng Yield (0.2% offset) |
35-65 MPa |
65-105 MPa | 95-135 MPa | 125-165 MPa | ≥150 MPa |
| Pagpahaba sa Break |
18-25% |
8-14% | 6-12% | 4-10% | 3-8% |
| Katigasan (Rockwell B) |
25-40 |
40-55 | 50-70 | 60-80 | 70-90 |
| Ari-arian ng haluang metal 8011 |
Halaga |
| Densidad |
2.7 g/cm³ |
| Punto ng Pagkatunaw |
643–657°C |
| Thermal Conductivity |
209 W/m·K |
| Electrical Conductivity |
61% IACS |
| Thermal Expansion Coefficient |
23.1×10⁻⁶/°C (20–100°C) |
| ASTM |
B209 (sheet/plate), B221 (extrusions), B233 (wire), B479 (foil). |
| ISO |
ISO 26204 (alloy designations), ISO 6892 (mechanical testing). |
| UNS |
A91060 (United States Numbering System). |